Table Of Gauges
厚度对照表
| No. |
S.W.G (imperial Regal Standard Wire Gauge) |
U.S.S.W.G. or A.S.W.G. (United States Steel Wire Gauge) |
B.G. (British Standard Gauge or Birmingham Steel and Iron Gauge) |
J de P (Paris Gauge) |
B.W.G. (Birmingham Wire Gauge or Stubs Iron Wire Gauge) |
B.S. (Brown and Shape of American Standard) |
U.S.G. (U.S Standard for Plate) |
G.S.G. (Galvanized Sheet Gauge) For Hot-Dipped Zinc Coated Sheets |
||||||||
| in | mm | in | mm | in | mm | in | mm | in | mm | in | mm | in | mm | in | mm | |
|
15/0 14/0 13/0 12/0 11/0 10/0 9/0 8/0 7/0 6/0 5/0 4/0 3/0 2/0 0 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 |
- - - - - - - - 0.500 0.464 0.432 0.400 0.372 0.348 0.324 0.300 0.276 0.252 0.232 0.212 0.192 0.176 0.160 0.144 0.128 0.116 0.104 0.092 0.080 0.072 0.064 0.056 0.048 0.040 0.036 0.032 0.028 0.024 0.022 0.020 0.018 0.0164 0.0148 0.0136 0.0124 0.0116 0.0108 0.0100 0.0092 0.0084 0.0076 0.0068 0.0060 0.0052 0.0048 0.0044 0.004 0.0036 0.0032 0.0028 0.0024 0.002 0.0016 0.0012 0.001 - - |
- - - - - - - - 12.700 11.785 10.973 10.160 9.449 8.839 8.229 7.620 7.010 6.401 5.893 5.385 4.877 4.470 4.064 3.658 3.251 2.946 2.642 2.337 2.032 1.829 1.626 1.422 1.219 1.016 0.914 0.812 0.711 0.610 0.559 0.508 0.457 0.417 0.376 0.345 0.315 0.295 0.274 0.254 0.234 0.213 0.193 0.173 0.152 0.132 0.122 0.112 0.106 0.091 0.081 0.071 0.061 0.051 0.041 0.031 0.025 - - |
- - - - - - - - 0.049 0.462 0.430 0.394 0.362 0.331 0.306 0.283 0.262 0.244 0.225 0.207 0.192 0.177 0.162 0.148 0.135 0.120 0.106 0.092 0.080 0.072 0.062 0.054 0.048 0.041 0.035 0.0317 0.0286 0.0258 0.0230 0.0204 0.0181 0.0173 0.0162 0.0150 0.0140 0.0132 0.0128 0.0118 0.0104 0.0095 0.0090 0.0085 0.0080 0.0075 0.0070 0.0066 0.0062 0.0060 0.0058 0.0055 0.0052 0.0050 0.0048 0.0046 0.0044 - - |
- - - - - - - - 12.45 11.73 10.92 10.01 9.19 8.41 7.77 7.19 6.65 6.20 5.72 5.26 4.88 4.50 4.11 3.76 3.43 3.05 2.69 2.34 2.03 1.83 1.57 1.37 1.22 1.04 0.890 0.805 0.726 0.655 0.584 0.518 0.460 0.439 0.411 0.381 0.356 0.335 0.325 0.300 0.264 0.241 0.229 0.216 0.203 0.191 0.178 0.168 0.157 0.152 0.147 0.140 0.132 0.127 0.122 0.117 0.112 - - |
1.000 0.9583 0.9167 0.8750 0.8333 0.7917 0.750 0.7083 0.6666 0.625 0.5883 0.5416 0.500 0.4452 0.3964 0.3532 0.3147 0.2804 0.250 0.2225 0.1981 0.1764 0.1570 0.1398 0.1250 0.1113 0.0991 0.0882 0.0785 0.0699 0.0625 0.0556 0.0495 0.0440 0.0392 0.0349 0.03125 0.02782 0.02476 0.02204 0.01961 0.01745 0.015625 0.0139 0.0123 0.0110 0.0098 0.0087 0.0077 0.0069 0.0061 0.0054 0.0048 0.043 0.00386 0.00343 0.00306 0.00272 0.00242 0.00215 0.00192 0.00017 0.00152 0.00135 0.00120 0.00107 0.00095 |
25.4 24.34 23.28 22.23 21.17 20.11 19.05 17.99 16.93 15.88 14.94 13.76 12.70 11.31 10.07 8.971 7.993 7.122 6.350 5.652 5.032 4.481 3.988 3.551 3.175 2.827 2.517 2.240 1.994 1.775 1.588 1.412 1.257 1.118 0.9957 0.8865 0.7938 0.7066 0.6289 0.5598 0.4981 0.4432 0.3969 0.3531 0.3124 0.2794 0.2489 0.2210 0.1956 0.1753 0.1549 0.1372 0.1219 0.1092 0.09804 0.08712 0.07772 0.06909 0.06147 0.05461 0.04877 0.00432 0.03861 0.03429 0.03048 0.02718 0.02413 |
- - - - - - - - - - 0.0122(5P) 0.0133(4P) 0.0150(3P) 0.0165(2P) 0.0196(1P) 0.0236 0.0275 0.0314 0.0354 0.0393 0.0433 0.0472 0.0512 0.0551 0.0590 0.0630 0.0708 0.0787 0.0866 0.0944 0.1062 0.1181 0.1338 0.1535 0.1732 0.1929 0.2126 0.2322 0.2520 0.2756 0.2992 0.3228 0.3464 0.3700 0.3937 - - - - - - - - - - - - - - - - - - - - - - |
- - - - - - - - - - - - - 0.400 0.500 0.600 0.700 0.800 0.900 1.000 1.100 1.200 1.300 1.400 1.500 1.600 1.800 2.000 2.200 2.400 2.700 3.000 3.400 3.900 4.400 4.900 5.400 5.900 6.400 7.000 7.600 8.200 8.800 9.400 10.000 - - - - - - - - - - - - - - - - - - - - - - |
- - - - - - - - - - 0.500 0.454 0.425 0.380 0.340 0.300 0.284 0.259 0.238 0.220 0.203 0.180 0.165 0.148 0.134 0.120 0.109 0.095 0.083 0.072 0.065 0.058 0.049 0.042 0.035 0.032 0.028 0.025 0.022 0.020 0.018 0.016 0.014 0.013 0.012 0.010 0.009 0.008 0.007 0.005 0.004 - - - - - - - - - - - - - - - - |
- - - - - - - - - - 12.70 11.53 10.80 9.65 8.64 7.62 7.21 6.58 6.05 5.59 5.16 4.57 4.19 3.76 3.40 3.05 2.77 2.41 2.11 1.83 1.65 1.47 1.24 1.07 0.89 0.81 0.71 0.64 0.56 0.51 0.46 0.41 0.36 0.33 0.30 0.25 0.23 0.20 0.18 0.13 0.10 - - - - - - - - - - - - - - - -
|
- - - - - - - - - - - 0.4600 0.4096 0.3648 0.3249 0.2893 0.2576 0.2294 0.2043 0.1819 0.1620 0.1443 0.1285 0.1144 0.1019 0.09074 0.08081 0.07196 0.06408 0.05707 0.05082 0.04526 0.04030 0.03589 0.03196 0.02846 0.02535 0.02257 0.02010 0.01790 0.01594 0.01420 0.01264 0.01126 0.01003 0.008928 0.007950 0.007080 0.006304 0.005614 0.0050 0.004453 0.003965 0.003531 0.003144 - - - - - - - - - - - - |
- - - - - - - - - - - 11.68 10.40 9.27 8.252 7.348 6.543 5.827 5.189 4.620 4.115 3.665 3.264 2.906 2.588 2.304 2.052 1.829 1.628 1.450 1.290 1.151 1.024 0.912 0.813 0.724 0.643 0.574 0.511 0.455 0.404 0.361 0.320 0.287 0.254 0.227 0.202 0.180 0.160 0.143 0.127 0.113 0.101 0.090 0.080 - - - - - - - - - - - -
|
- - - - - - - - 0.5000 0.46875 0.4375 0.40625 0.375 0.3437 0.3125 0.2813 0.2656 0.2500 0.2344 0.2188 0.2031 0.1875 0.1719 0.1563 0.1406 0.1250 0.1094 0.0937 0.0781 0.0703 0.0625 0.0563 0.0500 0.0438 0.0375 0.0344 0.0313 0.0281 0.0250 0.0219 0.0188 0.0172 0.0156 0.0141 0.0125 0.0109 0.0102 0.0094 0.0086 0.0078 0.0070 0.00664 0.00625 - - - - - - - - - - - - - - |
- - - - - - - - 12.700 11.906 11.113 10.319 9.525 8.730 7.938 7.145 6.746 6.350 5.954 5.558 5.159 4.763 4.366 3.970 3.571 3.175 2.779 2.380 1.984 1.786 1.588 1.430 1.270 1.113 0.953 0.874 0.795 0.714 0.635 0.556 0.478 0.437 0.396 0.358 0.318 0.277 0.259 0.239 0.218 0.198 0.178 0.169 0.159 - - - - - - - - - - - - - - |
- - - - - - - - - - - - - - - - - - - - - - 0.1681 0.1532 0.1382 0.1233 0.1084 0.0934 0.0785 0.0710 0.0635 0.0575 0.0516 0.0456 0.0396 0.0366 0.0336 0.0306 0.0276 0.0247 0.0217 0.0202 0.0187 0.0172 0.0157 0.0142 0.0134 - - - - - - - - - - - - - - - - - - - - |
- - - - - - - - - - - - - - - - - - - - - - 4.27 3.89 3.51 3.13 2.75 2.37 1.99 1.80 1.61 1.46 1.31 1.16 1.01 0.930 0.853 0.777 0.701 0.627 0.551 0.513 0.475 0.437 0.399 0.361 0.340 - - - - - - - - - - - - - - - - - - - - |